Laboratory Testing & General Mineral Processing Engineering

Laboratory Testing & General Mineral Processing Engineering

  • To participate in the 911Metallurgist Forums, be sure to JOINLOGIN
  • Use Add New Topic to ask a New Question/Discussion about Mineral Processing or Laboratory Work.
  • OR Select a Topic that Interests you.
  • Use Add Reply = to Reply/Participate in a Topic/Discussion (most frequent).
    Using Add Reply allows you to Attach Images or PDF files and provide a more complete input.
  • Use Add Comment = to comment on someone else’s Reply in an already active Topic/Discussion.

Slurry Lime Strength Test (4 replies)

G
Teggry
1 year ago
Teggry 1 year ago

Hi,

I'm looking to writing up a procedure on Lime Slurry Strength test.

Can anyone run through what the steps are please?

J
Jorge
1 year ago
Jorge 1 year ago

You can use the sugar procedure to determine the CaO content

J
Jorge
1 year ago
Jorge 1 year ago

%CaO =  (28 x mL (HCl) x N(HCl))/mg (sample)

J
Jorge
1 year ago
Jorge 1 year ago
1 like by David

The main steps are below

- Take a representative sample and dry it. Homogenize and take 150 g to pulverize

- Homogenize the pulverized material and take 0.5 g

- Add 10 mL of distilled water in a 250 mL Erlenmeyer Flask. Add the 0.5 g, mix and add 50 mL og distilled water

- Heat and boil the system for 5 minutes. Remove tbe flask 

- When the flask is cold, add 50 mL of distilled water, mix the system and add 15 to 18 grams of sugar. The reaction take 15 minutes

- Add 4 to 5 drops of indicator. The titration agent is HCl

- Once the final is reached (the solution has not pink color), observe the mL of HCl added and use the formula

 

 