Metallurgists Need Statistics

VARIABLE

RANGE

EFFECT ON PROCESS

Crushing

Jaw Crusher Close side setting

3″ plus

– Material too large for cone crusher.

N – 3″

L – Reduction in capacity. Excess power draw.

Cone Crusher Close side setting

3/8″ – 1″

H – Increased circulating load of screen and cone.

N – 1/2″

L – Increased power consumption, decrease capacity.

Dust Collector recirculating % solids

7 – 10%

H– Excessive nozzle and impeller wear.

N – 8%

L – No effect.

Grinding

 Mill Feed Conveyor Speed (feed rate)               0-33 mtph  H– May overload mill with increase in circulating load.
 N – 22 mtph
 L – Decrease in plant
throughput.
 Mill Percent solids  50-70%  H-Increase in circulating load. Poor grinding efficiency.
 N – 60%
 L – Increase throughput but decreases grinding efficiency
 Cyclone Feed Density  45 – 60%  H– Coarse particles in
cyclone overflow.
 N – 52% solids.
 L – Fine particles in cyclone overflow, less product.
 Cyclone 0/F density  25 – 35% H– Coarse particle in cyclone overflow, potential to sand gravity line to thickener.
 N – 30%
 L – Fine particles in cyclone overflow.
 Cyclone Apex opening  2 “-4” – Decrease cyclone underflow density.
 N – As required.
 L – Increase cyclone underflow density and potential ‘roping’ condition.
 Cyclone 0/F pH  10-11  – Waste of lime.
 N – 10.5
 L – Danger of HCN generation.
 Cyclone U/F density  60-75%  – Coarse particles in cyclone overflow and increase in circulating load.
 N – 69%
 L – Fine particles in cyclone underflow, less product.
 Thickening
 Thickener Overflow clarity  15-100 ppm  – Increase load on clarifier
 N – 50 ppm.
 L – Good.
 Thickener Underflow solids  50-70%  – Potential for sanding lines.
 N – 60%
 L – Excess pregnant solution in leach feed.
 Thickener Flocculant addition  25-100 gm/t – Waste of flocculant and underflow could become jelly-like.
 N – 50 gm/tonne.
 L – Solids increase in thickener overflow.
 Leaching
 Leaching Cyanide concentration 5-9 kg/tonne  – Waste of cyanide, may dissolve undesirable metals.
N – 7 kg/tonne
 L – Incomplete precious metals dissolution.
Leaching Air addition  2-3 kg/tonne  – Wasting lime.
N – 2.55 kg/tonne
 L – HCN generation, incomplete precious metals dissolution.
 Leaching Pulp density  40-50%  – Excess power required to keep slurry in suspension, solids may scale.
 N – 45%
L – Decrease in retention time, hence recovery.
 Filtration
 Filtration Filter feed pH  11.5-12.5  – Waste of lime.
 N – 12.0
 L – Poor filtration, slimly cake and reduced throughput.
 Filtration Vacuum 18-25″ Hg  – Wasting energy.
 N – 22″ Hg
 L – Increase in cake moisture, poor pregnant solution recovery, slimly cake.
 Filtration Flocculant addition  50-100 gm/tonne  – Waste of flocculant.
 N – 75 gm/tonne
 L – Blinding of filter cloth.
 Flotation
 Flotation Air  – Will float waste (gange) material.
 N – 100/30 S C F M rougher/cleaner cells.
 L – Poor froth generation and recovery.
 Merrill-Crowe
 Deaeration Vacuum  18-25″ Hg  – Waste of energy.
  N – 22″ Hg
 L – Poor removal of oxygen from solution, gold/silver will redissolve.